Materials
Cadmium oxide (CdO, 99.99%, Aldrich), octadecylphosphonic acid (ODPA, 99%, PCI), trioctylphosphine oxide (TOPO, 99%, Aldrich), trioctylphosphine (TOP, 97%, Aldrich), diphenylphosphine (DPP, 98%, Aldrich), selenium (Se, 200 mesh, 99.999%, Alfa Aesar), 1-octadecene (ODE, 90%, Aldrich), oleic acid (OA, 90%, Aldrich), oleylamine (OAm, 70%, Aldrich), manganese(II) acetate tetrahydrate (Mn(ac)2·4H2O, 99.999%, Strem) and tributylphosphine (TBP, 95%, Aldrich) were used as received.
Synthesis of Mn-doped core/shell CdSe/CdS QDs
Synthesis of CdSe cores
CdSe core particles with a wurtzite crystal structure were synthesized following a previously reported method17. Specifically, 100 mg of CdO, 490 mg of ODPA and 5 g of TOPO were loaded into a three-neck flask and degassed under vacuum at 150 °C for 1 h. Under nitrogen flow, the mixture was heated to 320 °C and maintained at this temperature until it formed a clear solution. Subsequently, 1 ml of TOP was swiftly injected into the flask. After the temperature increased to 380 °C, 1 ml of a 1.4 M TOP–Se solution was rapidly injected. At this stage, 1 mol% of DPP was added to the TOP–Se solution to control the growth kinetics17. After 3 min, the reaction mixture was cooled to room temperature by removing the heating mantle.
The resulting nanocrystals were collected by adding ethanol followed by centrifugation at 8,000 rpm. This washing procedure was repeated three times. The purified nanocrystals were then redispersed in toluene.
Mn doping
To incorporate Mn into the synthesized CdSe nanocrystals, we used a diffusion-doping procedure16 following a refined protocol of ref. 17. To remove residual Cd species, the pre-synthesized CdSe nanocrystals dispersed in toluene were precipitated with ethanol. 75 mg of the precipitate was dissolved in a mixture of 27 ml of degassed ODE and 2.7 ml of OA. The mixture was heated to 60 °C under vacuum for 1 h. After cooling to room temperature, the nanocrystals were again precipitated with ethanol and collected by centrifugation at 8,000 rpm. The resulting precipitate was added to a mixture of 510 mg of Se, 3 ml of degassed ODE and 3 ml of TBP.
Separately, 90 mg of Mn(ac)2·4H2O, 45 ml of ODE, 1.8 ml of OA and 3.9 ml of OAm were loaded into a flask and degassed under vacuum at 100 °C for 1 h. Under nitrogen flow, the mixture was heated to 300 °C, after which the previously prepared CdSe nanocrystal/TBP–Se solution in ODE was swiftly injected. The reaction temperature was maintained at 300 °C and the doping level was controlled by the reaction time (typically 5–30 min). After completion of the reaction, the mixture was cooled to room temperature. Magnetic circular dichroism measurements indicated approximately 2–5 internal Mn2+ dopants per QD, depending on the doping time17.
CdS shell growth
Owing to the large abundance of surface trap states, as-prepared Mn-doped CdSe cores do not exhibit detectable PL. To suppress surface defects, the cores were coated with a CdS shell following procedures reported in ref. 17.
To prepare a Cd-oleate precursor solution, 123 mg of CdO, 2.45 ml of OA and 10.8 ml of ODE were loaded into a flask and degassed at 100 °C under vacuum for 1 h. Under nitrogen flow, the temperature was increased to 250 °C and maintained for 1 h until a clear solution formed. The precursor solution was then cooled to 100 °C and maintained at this temperature until injection during CdS shell growth.
A TOP–S precursor solution was prepared by stirring a mixture of 18 ml of TOP and 44.3 mg of sulfur powder overnight in a glovebox.
For shell growth, 75 mg of Mn-doped CdSe QDs were dissolved in a mixture of 28 ml of ODE, 2.4 ml of OAm and 1.2 ml of OA. This mixture was degassed at 100 °C under vacuum for 1 h. Under nitrogen flow, the flask was heated to 220 °C and 0.4-ml aliquots of the Cd-oleate and TOP–S precursor solutions were alternately injected dropwise at intervals of 2.5 min for two cycles.
Fabrication of Auston switch devices
A 100-nm gold layer was evaporated onto the backside of a 1-mm glass substrate to serve as the ground plane. An approximately 200-nm-thick film of undoped (reference) or Mn-doped CdSe/CdS QDs was then deposited on the top surface of the substrate through repeated spin-coating cycles, accompanied by ligand exchange and rinsing steps. During deposition, QDs dispersed in octane (20 mg ml−1) were spin-coated at 1,600 rpm for 30 s.
To facilitate interdot charge transport, the QDs were cross-linked by means of solid-state ligand exchange, replacing the original long-chain ligands with short bifunctional 1,2-ethanedithiol (EDT) molecules. For ligand exchange, 60 µl of a 1 M EDT solution in methanol (MeOH) was dropped onto the QD layer, allowed to soak for 60 s and then spin-coated at 1,200 rpm for 30 s.
The film was subsequently rinsed by spin-coating pure MeOH to remove excess ligands. These three steps—QD deposition, ligand exchange and rinsing—were repeated five times to obtain a QD layer approximately 200 nm thick. The resulting film was annealed at 150 °C for 30 min.
Finally, two 200-nm-thick gold contacts separated by a 70-µm gap were deposited on top of the QD film through a shadow mask. Together with the gold ground plane on the backside of the substrate, these contacts form a microstrip transmission line with a nominal impedance of 50 Ω.
To verify that ligand exchange and film fabrication preserved the quantum-confined electronic structure of the QDs, we performed further TA measurements on 200-nm-thick Mn-doped CdSe/CdS QD films prepared using the same ligand-exchange procedure as used for the TPC devices. The TA spectra of the film samples were compared with those of the corresponding QDs in solution under identical excitation conditions (3.6-eV, 150-fs excitation; ⟨N⟩ = 0.3). The results are presented in Extended Data Fig. 8.
To characterize the equilibrium electrical properties of the ligand-exchanged QD films, further dark-conductivity measurements were performed using 120-nm-thick Mn-doped CdSe/CdS QD films deposited on glass substrates and contacted by thermally evaporated interdigitated Au electrodes comprising 25 pairs of 2-mm-long fingers separated by 10 μm. The corresponding current–voltage characteristics are presented in Extended Data Fig. 2.
Electrostatic simulations of the Auston switch geometry were performed using the Electrostatics interface of COMSOL Multiphysics to calculate the electric-field distribution, effective gap capacitance and effective RC constant (Extended Data Fig. 1).
TA measurements
TA measurements were performed using a standard pump–probe set-up in which absorption changes induced by a short pump pulse were probed in both the temporal and spectral domains using variably delayed probe pulses. The TA system was built around a regeneratively amplified ytterbium-doped potassium gadolinium tungstate (Yb:KGW) femtosecond laser (PHAROS, Light Conversion) generating approximately 190-fs pulses at 1.2 eV.
The laser output was split into two beams. One beam seeded a harmonic generator (HIRO HHG, Light Conversion) to produce second (2.4-eV) or third (3.6-eV) harmonic pump pulses, whose duration was shortened to about 150 fs owing to nonlinear optical pulse compression. Pulses from the second beam were delayed relative to the pump using an optical delay line (up to 5 ns) and focused onto a 3-mm-thick sapphire plate to generate broadband probe pulses in the form of a femtosecond white-light continuum.
The pump beam was focused onto the sample into a spot with a diameter of about 120 µm, whereas the smaller-diameter probe beam (<90 µm) was centred near the middle of the pump spot. Probe pulses transmitted through the sample were detected using an Avantes AvaSpec-Fast ULS1350F-USB2 spectrometer. The measured TA spectra were corrected for chirp (spectrally dependent delay within the white-light continuum probe pulses) using the procedure described in ref. 2.
In Auger recombination studies of undoped and Mn-doped QDs, we monitored the pump-induced band-edge absorption bleach (ΔαBE), which tracks the decay of band-edge excitonic populations14.
TPC measurements
To minimize sample degradation during TPC measurements, the fabricated Auston switch devices were mounted in a nitrogen-filled, airtight chamber equipped with optical windows and electrical feedthroughs. Under these conditions, no measurable changes in the TPC response were observed during the complete characterization of a device, including pump-fluence-dependent, transport-distance-dependent and bias-dependent measurements.
The chamber was mounted on a translation stage, allowing the laser beam position within the electrode gap to be varied. One of the top gold electrodes was biased using a DC power supply (Keithley 2430), whereas the other electrode was connected to a 20-GHz-bandwidth sampling oscilloscope by means of a coaxial cable. To minimize timing jitter, the oscilloscope was triggered by electrical pulses generated by a high-speed Si photodetector driven by a portion of the laser beam split from the excitation path.
The QDs within the photoconductive gap of the Auston switch were excited at 2.4 eV or 3.6 eV using 150-fs pulses of the second or third harmonic of an amplified Yb:KGW femtosecond PHAROS laser, respectively. The laser beam was focused with a cylindrical achromatic lens into a narrow stripe aligned with the edges of the top gold electrodes. The spatial profile of the excitation beam was approximately Gaussian, with a stripe width of about 70–80 µm (FWHM), measured with a beam profiler. The excitation position within the photoconductive gap of the Auston switch was varied by translating the sample in a plane perpendicular to the laser beam. The position was initially calibrated using a beam profiler and monitored in real time on the sample with a CMOS camera.
As discussed in Supplementary Note 3, the nonlinear dependence of SE-Auger upconversion on excitation density narrows the lateral spatial profile of the mobile hot-electron population relative to the laser beam profile (Extended Data Fig. 9). Across the film thickness, the initial hot-electron population is weighted towards the illuminated surface. However, because the optical absorption length is comparable with the QD film thickness, excited Mn ions are generated throughout the layer. Consequently, SE-Auger regeneration remains active across the film thickness, even if the hot-electron population spreads vertically during transit within the photoconductive gap.